标准 |
牌号 |
抗拉强度 (Mpa) |
屈服强度 (Mpa) |
伸长率(%) |
|
纵向 |
横向 |
||||
GB/T1898 -2003 |
16MnDG |
490-665 |
≥325 |
≥30 |
-- |
10MnDG |
≥400 |
≥240 |
≥35 |
-- |
|
09DG |
≥385 |
≥210 |
≥35 |
-- |
|
09Mn2VDG |
≥450 |
≥300 |
≥30 |
-- |
|
06Ni3MoDG |
≥455 |
≥250 |
≥30 |
-- |
|
ASTM A333 |
Grade1 |
≥380 |
≥205 |
≥35 |
≥25 |
Grade3 |
≥450 |
≥240 |
≥30 |
≥20 |
|
Grade4 |
≥415 |
≥240 |
≥30 |
≥16.5 |
|
Grade6 |
≥415 |
≥240 |
≥30 |
≥16.5 |
|
Grade7 |
≥450 |
≥240 |
≥30 |
≥22 |
|
Grade8 |
≥690 |
≥515 |
≥22 |
-- |
|
Grade9 |
≥435 |
≥315 |
≥28 |
-- |
|
Grade10 |
≥550 |
≥450 |
≥22 |
-- |
|
Grade11 |
≥450 |
≥240 |
≥18 |
-- |
级别 |
最低冲击试验温度 |
|
℉ |
℃ |
|
16MnDG |
-- |
-45 |
10MnDG |
-- |
-45 |
09DG |
-- |
-45 |
09Mn2VDG |
-- |
-70 |
06Ni3MoDG |
-- |
-100 |
A333 Grade1 |
-50 |
-45 |
A333 Grade3 |
-150 |
-100 |
A333 Grade4 |
-150 |
-100 |
A333 Grade6 |
-50 |
-45 |
A333 Grade7 |
-100 |
-75 |
A333 Grade8 |
-320 |
-195 |
A333 Grade9 |
-100 |
-75 |
A333 Grade10 |
-75 |
-60 |
A333 Grade11 |
-- |
-- |
为了让低温管有适用价值,必需给它增添别的金属作为参谋。 监视气体也使不得保证能需要一度彻底被气体密闭的条件,终究工人在细工焊接时,拳套还是要接触GB/T18984_2003低温管。关于一些特殊状况,比方说焊接全体较大,为了优化频率,也会运用电弧来充任气体条件。
由于它必需被隔离,而后再停止高贵而又简单的化学岁序。
PAW,这种方法临时没有应用来自天车打造,次要用来军工。
TIG(Tungstene Inert Gas 惰性钨气体焊接),这种焊接方法在上回给王木土的Lapierre材料中谈到过。 MIG(Metal Inert Gas 惰性金属气体焊接),它运用的是线圈状的可熔栅极。
这所有的大前提是依据钛自身固部分本质去做。 一只钛合金井架,用取相近值的姿态来看待。因为,一般所称的“钛”,它是一种有着特殊本质的合金。有两种方法来创举一度焊接条件,第一种方法是运用一度钟形罩,另一种方法是在焊接位置保持需要一种惰性气体,要求源源一直,流量丰盛,延续稳固,用气旋将整个条件覆盖。正常选用氩气和氦气,由于它们简单被需要,并且价格廉价。称之为沉浸式凝结。有六角形或者许正方体。
钛极难提炼。固然GB/T18984_2003低温管钛的六角形结晶体结构使其本质优异,然而量度能让此结构有所改观(那里是化学变迁,跟后面所讲的热收缩,热传播等物理变迁不归于同一范围)。 次要的焊接技能有三种,都是采纳电弧。
为了减小某个反应,好点的GB/T18984_2003低温管焊接替务间都会先污染气氛条件,并且会在这时间内冲入少量的中性气体。从总的观念来看,钛的精彩取决它有很高的强度,品质比(强度高,然而品质轻),优良的抗腐蚀性,非磁性。那里采纳的是一种用钨做丝的不行熔栅极。在焊接的小条件里,这种气体时惰性的。此外,采纳气体被称为“监视气体”。热收缩和热传播系数小,抗冲锋陷阵韧性(国际部分车友称之为金属复原性)和抗疲倦指数初等次要特性。
对于GB/T18984_2003低温管材停止焊接,否则,在钛管的焊接报外部会涌现裂口。在用量下面,是将75%的氩气和25%的氦气混合。假如把钛适用于轻工业中,钛对于冲突带来的消耗很迟钝。容易举例就是,在高速中,链条对于一片纯钛飞轮的磨损,就像焊接GB/T18984_2003低温管时发生的反响这样猛烈。由于某个原因,把钛称为饱满结晶体结构,因而钛合金中不行以有小半的杂质,哪怕是很小的含量。纯钛象征着什么也不是,由于它太坚硬了。在焊接的时分,高温的条件下,要把一切危险的范畴用气体隔离,使之不被杂质“沾染”。资料学上,咱们称钛合金为同素异形金属,由于它能出现出相反的结晶体外形。
材料牌号: 45 材料名称: 优质碳素钢 标 准 号: GB699-88 试样尺寸: 25 试样状态: 退火钢 抗拉强度: ≥600 (MPa) 屈服强度: ≥355 (MPa) 延 长 率: ≥16...
抗拉强度 σb (MPa):≥500伸长率 δ10 (%):≥25注 :板材的拉伸力学性能试样尺寸:厚度0.5~15热处理规范:热加工温度730~820℃;退火温度600~670℃。
1、屈服点:又称为屈服强度,在钢筋混凝土结构设计中所用的钢筋标准强度就是以钢筋屈服点为取值依据的。 2、抗拉强度:指钢筋抵抗拉力破坏作用的最大能力。 3、伸长率:义称延伸率,是指钢筋受拉力作用至断...
低温管道用无缝钢管
产品规格:8-1240×1-200mm<1/8”—48”×SCH5S—SCH160、STD、XS、XXS>
产品材质:16MnDG、10MnDG、09DG、09Mn2VDG、06Ni3MoDG、
ASTM A333-Grade1、Grade3、Grade4、Grade6、Grade7、Grade8、Grade9、
Grade10、Grade11
标准 |
牌号 |
化学成分(%) |
||||||||||
C |
Si |
Mn |
P |
S |
Cr |
Ni |
Cu |
Mo |
V |
Al |
||
GB/T18984 -2003 |
16MnDG |
0.12-0.20 |
0.20-0.55 |
1.20-1.60 |
≤0.025 |
≤0.025 |
-- |
-- |
-- |
-- |
-- |
-- |
10MnDG |
≤0.13 |
0.17-0.37 |
≤1.35 |
≤0.025 |
≤0.025 |
-- |
-- |
-- |
-- |
≤0.07 |
-- |
|
09DG |
≤0.12 |
0.17-0.37 |
≤0.95 |
≤0.025 |
≤0.025 |
-- |
-- |
-- |
-- |
≤0.07 |
-- |
|
09Mn2VDG |
≤0.12 |
0.17-0.37 |
≤1.85 |
≤0.025 |
≤0.025 |
-- |
-- |
-- |
-- |
≤0.12 |
-- |
|
06Ni3MoDG |
≤0.08 |
0.17-0.37 |
≤0.85 |
≤0.025 |
≤0.025 |
-- |
2.5-3.7 |
-- |
0.15-0.30 |
≤0.05 |
-- |
|
ASTM A333 |
Grade1 |
≤0.30 |
-- |
0.40-1.06 |
≤0.025 |
≤0.025 |
-- |
-- |
-- |
-- |
-- |
-- |
Grade3 |
≤0.19 |
0.18-0.37 |
0.31-0.64 |
≤0.025 |
≤0.025 |
-- |
3.18-3.82 |
-- |
-- |
-- |
-- |
|
Grade4 |
≤0.12 |
0.18-0.37 |
0.50-1.05 |
≤0.025 |
≤0.025 |
0.44-1.01 |
0.47-0.98 |
0.40-0.75 |
-- |
-- |
0.04-0.30 |
|
Grade6 |
≤0.30 |
≥0.10 |
0.29-1.06 |
≤0.025 |
≤0.025 |
-- |
-- |
-- |
-- |
-- |
-- |
|
Grade7 |
≤0.19 |
0.13-0.32 |
≤0.90 |
≤0.025 |
≤0.025 |
-- |
2.03-2.57 |
-- |
-- |
-- |
-- |
|
Grade8 |
≤0.13 |
0.13-0.32 |
≤0.90 |
≤0.025 |
≤0.025 |
-- |
8.40-9.60 |
-- |
-- |
-- |
-- |
|
Grade9 |
≤0.20 |
-- |
0.40-1.06 |
≤0.025 |
≤0.025 |
-- |
1.60-2.24 |
0.75-1.25 |
-- |
-- |
-- |
|
Grade10 |
≤0.20 |
0.10-0.35 |
1.15-1.50 |
≤0.030 |
≤0.015 |
≤0.15 |
≤0.25 |
≤0.015 |
≤0.50 |
≤0.12 |
≤0.06 |
|
Grade11 |
≤0.10 |
≤0.035 |
≤0.60 |
≤0.025 |
≤0.025 |
≤0.50 |
35.0-37.0 |
-- |
≤0.50 |
-- |
-- |
低温管理论重量计算公式:(外径-壁厚)×壁厚×0.02466=KG/M(每米的重量)
船用集装箱锁具中的锁轴原为 4 5钢 ,在低温 ( - 2 0℃ )下其性能尤其是冲击值达不到用户 2 7J的要求 ,航行时容易产生脆断。选用Q345钢 ,通过采用适当的锻造工艺和热处理工艺 (正火处理 ) ,锁轴拉伸、冲击性能在低温下使用有了很大的改善 ,延长了使用寿命 ,满足了用户的要求。
厚板钢材在高层建筑和大跨结构中得到了广泛应用,然而厚度的增加会引起钢板力学性能的变化,特别是厚度方向的性能。采用圆棒拉伸试样,对厚度为60~150mm的建筑结构用厚板Q345B进行了低温力学性能试验,试样分为垂直轧制方向的横向试样和贯穿厚度方向的Z向试样。试验获得了4种厚度钢板的屈服强度fy、抗拉强度fu和断面收缩率ψ等指标及其随温度和取样位置的变化关系,并测得4种厚度钢板Z向性能的相应指标。试验结果表明,随温度的降低,厚板的屈服强度和抗拉强度增大而断面收缩率减小;由钢板表面至中心,横向试样的断面收缩率呈下降趋势;随钢板厚度的增加,Z向试样的断面收缩率逐渐减小,且小于横向试样的断面收缩率。
执行标准
A333-1.6
A334-1.6
A333-7.9
A334-7.9
A333-3.4
A334-3.4
A333-8
A334-8
G3460
G3464
SEW680
低温钢管简介
低温钢管
低温管道用无缝钢管
现货规格:8-1240×1-200mm<1/8”—48”×SCH5S—SCH160、STD、XS、XXS>
产品材质:、10MnDG、09DG、09Mn2VDG、06Ni3MoDG、
ASTM A333-Grade1、Grade3、Grade4、Grade6、Grade7、Grade8、Grade9、
Grade10、Grade11
产品应用:适用于-45℃~-195℃级低温压力容器管道以及低温热交换器管道用无缝钢管
生产工艺:冷拔和热轧
重量计算公式:(外径-壁厚)*壁厚*0.02466/1000=米/吨
低温管道用无缝钢管
现货规格:8-1240×1-200mm<1/8”—48”×SCH5S—SCH160、STD、XS、XXS>
执行标准:GB/T18984-2003、ASTM A333
产品材质:16MnDG低温管、10MnDG低温管、09DG低温管、09Mn2VDG低温管、06Ni3MoDG低温管、
ASTM A333Gr1低温管、A333Gr3低温管、A333Gr4低温管、A333Gr6低温管、A333Gr7低温管、A333G8低温管、A333Gr9低温管、
A333Gr10低温管、A333Gr11低温管
产品应用:适用于-45℃~-195℃级低温压力容器管道以及低温热交换器管道用无缝钢管